I've been casting boolits out of this mold for a few weeks now.
Here are a few of my pointers please add anything of value you might have.
#1 It is by far the hardest mold, to get good boolits out of, I have ever had.
#2 Mold Temp has to be over 200 degrees using a non contact thermometer on the Aluminum mold.
( I know it is not accurate on reflective surfaces but it gives me a number to work with)
#3 I have had much better luck with reduced flow out of my Lee 4-20 pot
#4 Higher flow rate trapped more air and gave me wrinkled boolits
#5 I have my PID set at 710 degrees which gives me 680 degrees on my thermometer
What do you do to get good boolits out of this mold ??