    Quote Originally Posted by clodhopper View Post
    I'm using paste flux for soldering copper pipe applied with a Qtip.
    Standing all the jackets made from fired brass up right in a stainless steel pan and putting them on an electric burner.
    Okay todays experiments show this to only bond 50% or so of parts.
    Tin sounds like a good solution, at least I have some handy.
    To lazy to chase arrows.
    Clodhopper

  2. #22
    Boolit Buddy


    Join Date
    Apr 2009
    Location
    Cleveland, OH
    Posts
    427
    Not sure why you want to reinvent the wheel. Just buy corbin's flux, use a drop per core and be done with it. It never fails in my experience. A quart will last you several lifetimes.
    Zbench

  3. #23
    Boolit Master

    Join Date
    Feb 2008
    Location
    Bozoland Mt.
    Posts
    1,698
    Key word "buy"
    To lazy to chase arrows.
    Clodhopper

  4. #24
    Boolit Buddy
    hardcase54's Avatar
    Join Date
    Nov 2009
    Location
    Virginia
    Posts
    276
    Corbin's is all I have ever used, has not failed yet.
    " CANCER SUCKS" I swage .224, 6mm, 7mm, .308, 9mm, .40, .429. Also 9 to 30 jackets, and 9 to 9 jackets.

  5. #25
    Banned

    Join Date
    Dec 2007
    Location
    soda springs Id.
    Posts
    28,088
    seating the cores before the heat could help since you wouldn't have a lot of air there to release the flux.
    I have been melting mine like I described then core seating.

    I could try the flux in the jacket, then core seating, then do the melt.

    I have been doing the melt because it seems to help fill out the jacket better in the point form die and because I can get about 2 more grains of core weight in there.

  6. #26
    Boolit Buddy uncle dino's Avatar
    Join Date
    Apr 2015
    Location
    thumb of Mi.
    Posts
    432
    R5R..I,would advise against seating core before bonding..they do pop..I've had cores hit the lid of pot even when I've had plenty of clearance to let gases, moisture or whatever escape. When core lets go it splatters lead all over the outside of jackets of surrounding bullets. Zbench called it...I also would highly recommend Corbin's core bond..it really works great..lasts forever. Any little bit of impurities left in jacket will float right to the top.. 2 oz. is 8 bucks and will probably do thousands of bullets?. D
    Last edited by uncle dino; 03-06-2017 at 11:06 PM.

  7. #27
    Banned

    Join Date
    Dec 2007
    Location
    soda springs Id.
    Posts
    28,088
    thanks Dino.
    i'll probably just break down and get some.
    I know how important a flux is to cleaning before bonding when soldering, and my cores get pretty oxidized after cleaning the swage lube off them.

  8. #28
    Boolit Master

    Join Date
    Feb 2008
    Location
    Bozoland Mt.
    Posts
    1,698
    I checked Corbin's web site today, Core bond seem to be out of stock.
    To lazy to chase arrows.
    Clodhopper

  9. #29
    Boolit Buddy uncle dino's Avatar
    Join Date
    Apr 2015
    Location
    thumb of Mi.
    Posts
    432

  10. #30
    Boolit Master

    Join Date
    Feb 2008
    Location
    Bozoland Mt.
    Posts
    1,698
    Thanks Dino, that's not the same page I found it on yesterday.
    Corbin's web site is such a warren, all kinds of jems hiding in it.
    To lazy to chase arrows.
    Clodhopper

  11. #31
    Boolit Buddy


    Join Date
    Apr 2009
    Location
    Cleveland, OH
    Posts
    427
    A word of advise, when you do use that flux and heat the assembled core and bullet, some of the flux will fizz out and spray on the surroundings. It will rust steel in a heartbeat, so make sure you have anything you care about covered up. I use aluminum foil.
    Zbench

  12. #32
    Boolit Buddy Faret's Avatar
    Join Date
    Jan 2009
    Location
    South Central Wisconsin
    Posts
    472
    Quote Originally Posted by Zbench View Post
    A word of advise, when you do use that flux and heat the assembled core and bullet, some of the flux will fizz out and spray on the surroundings. It will rust steel in a heartbeat, so make sure you have anything you care about covered up. I use aluminum foil.
    Would this do any damage to the heating elements on a electric kiln or furnace?

  13. #33
    Boolit Buddy PWS's Avatar
    Join Date
    Dec 2010
    Location
    Kodiak, AK
    Posts
    266
    Quote Originally Posted by uncle dino View Post
    Ordered some today too, Thanks Dino!

  14. #34
    Boolit Buddy


    Join Date
    Apr 2009
    Location
    Cleveland, OH
    Posts
    427
    I don't think so. One thing needed for rust is moisture, which is in precious supply at 1000 F!
    Zbench

  15. #35
    Banned

    Join Date
    Dec 2007
    Location
    soda springs Id.
    Posts
    28,088
    my little heater element was 10$ at the walmart.
    I could probably absorb that financial set-back if it gets ruined.

  16. #36
    Boolit Buddy uncle dino's Avatar
    Join Date
    Apr 2015
    Location
    thumb of Mi.
    Posts
    432
    I'm not sure about long term affects of core bond on enclosed heating elements.. I've only ran maybe 5 large batches in my kiln. I see scale on the elements.. But that may be normal..I find myself using a giant cast iron frying pan with a lid over a propane burner..Is a lot quicker..300 bullets in pan. Burner on high ..7-8 minutes..done. the few vapors from core bond seem to help keep oxidation on outside of jacket to a minimum..if you resist the temptation to take the lid off and peek..D

  17. #37
    Boolit Buddy PWS's Avatar
    Join Date
    Dec 2010
    Location
    Kodiak, AK
    Posts
    266
    Holy Moley! Core Bond showed up yesterday and had a chance to try some. What a difference! The cores wetted to the jackets and everything performed the way Corbin's says. Proof is in the shooting but that'll be at least a few days.

    Core freshly melted and wetted to jacket:

    Click image for larger version. 

Name:	IMG_4129.jpg 
Views:	25 
Size:	40.5 KB 
ID:	190569

    Cores solidified and shrinkage hole showing that they're holding to the jacket:

    Click image for larger version. 

Name:	IMG_4127.jpg 
Views:	21 
Size:	64.1 KB 
ID:	190570

  18. #38
    Boolit Buddy uncle dino's Avatar
    Join Date
    Apr 2015
    Location
    thumb of Mi.
    Posts
    432
    I wet tumble the cores in baking soda and car wash after I bond...once you remove them from the wash, water will be trapped in the hole in center of core. I place all the cores back in pot @ 200 degrees for at least 1/2 hour to get water out.. Look real close when you core seat, if you can see the water on top of the core if it isn't dry enough..water will create voids in core otherwise...don't core seat without washing...will rust up your die.. D

  19. #39
    Banned

    Join Date
    Dec 2007
    Location
    soda springs Id.
    Posts
    28,088
    baking soda is a PH neutralizer and super cheap don't skip using it.

  20. #40
    Boolit Master reed1911's Avatar
    Join Date
    Nov 2013
    Posts
    799
    Yep! Baking soda is great and if you use the A&H fridge/freezer packs it is more or less free since you were going to throw it away anyhow. I use them in the soda blaster as well.
    Ron Reed
    Oklahoma City, OK

Page 2 of 2 FirstFirst 12

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Abbreviations used in Reloading

BP Bronze Point IMR Improved Military Rifle PTD Pointed
BR Bench Rest M Magnum RN Round Nose
BT Boat Tail PL Power-Lokt SP Soft Point
C Compressed Charge PR Primer SPCL Soft Point "Core-Lokt"
HP Hollow Point PSPCL Pointed Soft Point "Core Lokt" C.O.L. Cartridge Overall Length
PSP Pointed Soft Point Spz Spitzer Point SBT Spitzer Boat Tail
LRN Lead Round Nose LWC Lead Wad Cutter LSWC Lead Semi Wad Cutter
GC Gas Check